Free calculators

Welding calculators

The math welders and weld inspectors do by hand on the job: heat input, minimum preheat, fillet weld strength and size, the visual acceptance limits, filler metal and tension test coupons. Type sizes as fractions (3/16, 1-1/2) or decimals. Every result shows the formula and the code clause it comes from.

Heat input

Check a weld against the WPS's heat input limit from the volts, amps and travel speed you measure.

Or time a run:

30 kJ/in (1.18 kJ/mm)

At 10 in/min travel speed.

Heat input (kJ/in) = volts × amps × 60 ÷ (1,000 × travel speed in in/min), as in ASME IX QW-409.1(a). For a weave, measure travel along the weld, not across it.

Minimum preheat

The prequalified minimum preheat and interpass temperature from AWS D1.1, by steel category and the thickest part at the weld.

A36, A572 Gr 42/50, A992, A500, A53 Gr B, A588 and similar, welded with E7018 type electrodes, GMAW, FCAW or SAW.

50°F (10°C)

Minimum preheat and interpass temperature

Carbon equivalent from a mill cert

Enter the percentages from the mill test report. Leave out what isn't listed.

CE = C + (Mn + Si)/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, the formula in AWS D1.1's guide to preheat. The higher it is, the more prone the steel is to hydrogen cracking and the more preheat it needs; that guide uses it when the table doesn't fit.

AWS D1.1 prequalified minimum preheat and interpass temperature (Table 3.2 in the 2000 edition; renumbered in later editions). Steel below 32°F is warmed to at least 70°F. A WPS that calls for more wins.

Fillet weld strength

What an equal-leg fillet carries in shear, or the size it needs for a load.

22.27 kips

3.712 kips per inch × 6 in; throat 0.177"

Throat = leg × 0.707. ASD: 0.30 × FEXX on the throat (AWS D1.1, AISC). LRFD: 0.75 × 0.60 × FEXX. Weld metal only; the engineer checks the base metal and the connection.

Fillet weld size limits

The smallest fillet AWS D1.1 allows for the parts joined, and the largest along a plate edge.

Minimum 3/16"

Based on T = 3/8" (the thinner part).

Largest along the edge: 7/16"

1/4 in. and thicker: 1/16 in. less than the plate, unless the drawing says to build it out to full throat.

AWS D1.1 minimum fillet weld sizes (Table 5.8 in the 2000 edition): up to 1/4 in. → 1/8 (3/16 cyclically loaded); to 1/2 → 3/16; to 3/4 → 1/4; over 3/4 → 5/16. Largest along an edge: D1.1 2.4.5. Design size from the drawings governs when bigger.

Visual acceptance check

Undercut, undersized fillets and piping porosity against the AWS D1.1 visual inspection acceptance criteria.

✓ Within 1/32" for material under 1".

AWS D1.1 visual inspection acceptance criteria (Table 6.1 in the 2000 edition). Undercut on statically loaded work: 1/32 in. under 1 in. thick (1/16 for up to 2 in. in any 12 in.), 1/16 in. from 1 in. up. Undersize: 1/16 for welds up to 3/16, 3/32 for 1/4, 1/8 from 5/16, over no more than 10% of the length (none at girder web-to-flange ends).

Filler metal for a job

How much weld metal a job takes and how much rod or wire to buy.

Buy about 19.5 lb of filler

11.7 lb of weld metal over 100 ft (0.0313 sq in cross-section).

Weld metal (lb) = joint area × length × 0.2836 lb/cu in × (1 + extra). Filler = weld metal ÷ deposition efficiency. Pipe joints use the outside circumference. A starting point for ordering, not a guarantee.

Tension test coupon

Tensile strength of a reduced-section coupon from a PQR or welder test, and whether it passes.

Fill in the boxes above to see the answer.

Tensile strength = break load ÷ coupon area. ASME IX QW-153.1: at least the base metal's specified minimum, or no more than 5% below it if the coupon broke in the base metal outside the weld or fusion line.

These do the arithmetic; they don't replace the code. Code values were checked against AWS D1.1:2000, and table numbers and some limits change between editions, so check the edition your contract names. The WPS, the contract documents and the engineer of record have the final say.

How inspectors use these

Checking a weld against the WPS. Read the volts and amps off the machine or a clamp meter, time a run with your phone and enter the length welded. The heat input calculator gives kJ/in and kJ/mm and flags a reading over the WPS limit. The preheat calculator gives the AWS D1.1 prequalified minimum for the steel category and the thickest part at the weld, and adds the 70°F rule when the steel is below freezing.

Sizing and accepting fillets. The fillet strength calculator works out the throat and the shear the weld metal carries (ASD or LRFD), or the size needed for a load. The size-limits calculator gives the smallest fillet allowed for the parts joined and the largest along a plate edge. The visual acceptance check compares undercut, an undersized fillet or piping porosity with the D1.1 limits for statically loaded, cyclically loaded and tubular work.

Ordering and testing. The filler metal calculator turns a joint and a length (or a count of pipe joints) into pounds of weld metal and rod or wire to buy. The tension test calculator gives a coupon's tensile strength and checks it against ASME IX QW-153.1.

These calculators do the arithmetic; they don't replace the code. Values were checked against AWS D1.1:2000, and table numbers and some limits change between editions, so check the edition your contract names.

Keep the records, not just the math

Sentinel Nexus keeps weld maps on your 3D models, visual and NDT inspections with photos and signatures, repairs, welder qualifications with continuity alerts, the WPS/PQR library and one-tap report PDFs. It works offline on the job site.